The properties of electroless nickel including corrosion resistance are influenced by the type of alloy. This can be a low phosphorous nickel coating, a medium phosphorous nickel coating, a high nickel phosphorous coating or a nickel boron coating.
The table below outlines the various properties and nickel alloy type.
| Property / Level of alloy | High a | Mid a | Mid-Low a | Low a | Mid-Low Bb | Low Bb |
|---|---|---|---|---|---|---|
| % Phosphorous | 10 – 13 | 7 – 9 | 4 – 6 | 1 – 3 | – | – |
| % Boron | – | – | – | – | 3 – 5 | 0.2 – 1 |
| Deposit density Range (g/cm3) | 7.6 – 7.9 | 8.0 – 8.2 | 8.3 – 8.5 | 8.6 – 8.8 | 8.25 | 8.8 |
| Plating rate (µ/Hr) | 7.5 – 15 | 7.5 – 15 | 18 – 30 | 11 – 19 | – | – |
| Hardnessc,f | 400 – 525 | 500 – 600 | 625 – 750 | 725 – 800 | 650 – 750 | 600 – 700 |
| Rockwell C (Rc) Hardness | 41 – 46 | 45 – 51 | 53 – 59 | 57 – 61 | 54 – 59 | 51 – 56 |
| Hardness after heat treatc | 850-950 | 850-1000 | 850-1100 | 900-1100 | 1100-1200 | 500-600 |
| Taber wear indexe,f | 22 – 24 | 16 – 20 | 10 – 14 | 7 – 12 | 3 – 10 | 7 – 9 |
| Coefficient of thermal expansiong | 8 – 10 | 10 – 15 | 11 – 14 | 12 – 15 | – | – |
| Electrical resistivityh | 75 – 110 | 40 – 70 | 15 – 45 | 10 – 30 | 40 – 90 | 10 – 20 |
| Thermal conductivityi | 0.010 | 0.012 | 0.016 | 0.015 | – | |
| Tensile strength (MPa) | 650-900 | 800-1000 | 350-600 | 200-400 | – | – |
| Elongation | 1 – 1.25 | 0.5 – 1 | 0.5 -1 | 0.5 – 1.5 | 0.2 | – |
| Modulus of elasticity (GPa) | 55 – 70 | 50 – 65 | 45 – 65 | 55 – 65 | 120 | – |
| Melting rangeoC | 880-900 | 880-980 | 1100-1300 | 1250-1360 | 1040-1080 | 1350-1390 |
| Coercivity (Oe) | 0 | 1 – 8 | 10 -15 | 15 – 80 | – | – |
| Magnetic propertiesf | Non | Slightly | Magnetic | Magnetic | – | Weakly |
| Internal stressf | Neutral to comp | Slightly tensile | Slightly comp | Slightly tensile | Tensile | |
.
Deposit Thickness Formula For Chemically Applied Deposits:
T = ────────────────── = cm where
D (87.53cm²) (2.54cm²/in²)
W = Deposit weight in grams,
D = Deposit specific gravity in grams/cm³= 8.88g/cm³ for pure nickel deposits.
The values for E and M are required to accurately solve the Stoney Formula and the value M is required to solve the Deposit Stress Analyzer Formula.
M = EDeposit ÷ ESubstrate
Frequently, the increase that the Modulus of Elasticity effects on the internal deposit stress of electroless applied alloy coatings is not recognized. Numerous formulas for calculating the internal deposit stress of metallic deposits do not include a correction for the difference of the Modulus of Elasticity between the deposit and the substrate material. In such cases, the calculated result can be far from the actual value. Call the supplier of your electroless nickel alloy plating chemistry for the Modulus of Elasticity value of the deposit.
Note: how necessary it is to use the value for M to determine the actual internal deposit stress value in calculating results for the bent strip method or for the spiral contractometer method. Often the results are calculated without incorporating the correct value of E in these formulas by assuming that electroless nickel deposits have a Modulus of Elasticity similar to that of pure nickel deposits, or they fail to include the value for M in the equations altogether.